Classifications
BIS Classifications
Electrode Classification | Range of Tensile Strength N/mm2 | Minimum Yield stress N/mm2 | Minimum elongation | Temperature and the required Temp °C Impact strength Joules | |
EX-40XX | 410-540 | 330 | 16 | Not required | |
EX-41XX | 410-540 | 330 | 20 | 27 | 47 |
EX-42XX | 410-540 | 330 | 22 | 0 | 47 |
EX-43XX | 410-540 | 330 | 24 | -20 | 47 |
EX-44XX | 410-540 | 330 | 24 | -30 | 27 |
EX-50XX | 510-610 | 400 | 16 | Not required | |
EX-51XX | 510-610 | 400 | 18 | 27 | 47 |
EX-52XX | 510-610 | 400 | 18 | 0 | 47 |
EX-53XX | 510-610 | 400 | 20 | -20 | 47 |
EX-54XX | 510-610 | 400 | 20 | -30 | 27 |
EX-55XX | 510-610 | 400 | 20 | -40 | 27 |
EX-56XX | 510-610 | 400 | 20 | -46 | 27 |
AWS Classifications
AWS CLASSIFICATION | TYPE OF COVERING | TYPE OF CURRENT |
E 6010 | High cellulose sodium | DC + |
E 6011 | High cellulose potassium | AC/DC + |
E 6012 | High titania sodium | AC/DC - |
E 6013 | High titania potassium | AC/DC ± |
E 6020 | High iron oxide | AC/DC - |
E 6022 | High iron oxide | AC/DC ± |
E 6027 | High iron, oxide iron powder | AC/DC - |
E 7014 | Iron powder, titania | AC/DC ± |
E 7015 | Low hydrogen sodium | DC + |
E 7016 | Low hydrogen potassium | AC/DC + |
E 7018 | Low hydrogen potassium, iron powder | AC/DC + |
E 7024 | Iron powder, titania | AC/DC ± |
E 7027 | High iron oxide, iron powder | AC/DC - |
E 7028 | Low hydrogen potassium, Iron powder | AC/DC + |
E 7048 | Low hydrogen potassium, iron powder | AC/DC + |